Fillet welds and partial penetration butt welds are checked according to EN 1993-1-8. The strength of complete joint penetration (CJP) butt welds is assumed to be the same as the strength of the base metal, and such welds are not checked, except for the cases described in Butt welds.
Fillet welds
Design resistance
The plastic redistribution in welds is used to automatically avoid the stress singularities in weld elements to redistribute the stress further along the weld length. The strength of the weld approximately matches the hand calculation, and the stress is correctly distributed for complicated issues like welding to an unstiffened flange (EN 1993-1-8:2005 – 4.10; EN 1993-1-8:2024 – 6.10). The stress in the throat section of a fillet weld is determined according to EN 1993-1-8:2005 – 4.5.3.2 or EN 1993-1-8:2024 – 6.5.3.2 (directional method). Stresses are calculated from the stresses in weld element. Bending moment around the longitudinal weld axis is not taken into account.
Standard weld check (EN 1993-1-8:2005 – 4.5.3.2(6), Equation (4.1); EN 1993-1-8:2024 – 6.5.3.2(6), Equation (6.1))
Weld utilization
where:
- σw,Ed – equivalent stress in the weld
- σw,Rd – weld resistance
- βw – correlation factor (EN 1993-1-8 – Table 4.1)
- fu – ultimate strength, chosen as the lower of the two connected base materials or according to material chosen by user
- γM2 – safety factor (EN 1993-1-8 – Table 2.1; editable in Code setup)
- σ┴, τ┴, τ‖ – stresses in weld according to the figure below:

Weld material
The user can choose one of three types of weld material:
- Automatic – the ultimate strength and the correlation factor are taken from the weaker of the connected plates (smaller ).
- Standard welding material (a steel grade, e.g. S 355) – and are taken from the welding material.
- Filler material according to EN 1993-1-8:2024 – Table 6.2 (42, 46, 69, 89) – used in the alternative weld check. When the alternative weld check does not apply, and are taken from the weaker of the connected plates.
The correlation factor is assigned to each steel grade according to its name and the selected edition. The values for S420 and S460 differ between the editions. The conservative, higher value is by default in the material database. For steel grades not listed in the table of the selected edition, the highest value of that table is used conservatively: for EN 1993-1-8:2005 and for EN 1993-1-8:2024. If the two connected plates have the same ultimate strength but different steel grade names, the conservative value is used as well. For HISTAR steels, the values of ETA-10/0156 are used ( for HISTAR 355/355 L, for HISTAR 460/460 L).
Alternative weld check for high-strength steel (EN 1993-1-8:2024 only – 6.5.3.2(7), Equation (6.2))
The alternative weld check is used when all of the following conditions are met:
- EN 1993-1-8:2024 is selected,
- at least one of the connected plates is made of steel grade S460 or higher ( MPa for the thickness of the plate),
- a filler material from EN 1993-1-8:2024 – Table 6.2 is chosen as the weld material.
Otherwise, the standard weld check is used.
where:
- – ultimate strength of the weaker of the connected plates
- – ultimate strength of the filler material (EN 1993-1-8:2024 – Table 6.2)
- – modified correlation factor (EN 1993-1-8:2024 – Table 6.2)
| Filler material (EN ISO 18275) | 42 | 46 | 69 | 89 |
| [MPa] | 500 | 530 | 770 | 940 |
| [–] | 0.89 | 0.85 | 1.09 | 1.19 |
For filler materials different to those given in this table, but not higher than G89, the next larger value of should be taken conservatively.
Because the steel grade is assessed by the yield strength at the actual plate thickness, a thick plate of a high-strength steel grade may fall below 460 MPa, and the standard weld check is used.
All values required for check are printed in tables. Ut is the utilization of the most stressed element. Since plastic redistribution of stress in weld is used, it is the decisive utilization. Utc provides information about utilization along the weld length. It is the ratio of actual stress at all elements of the weld to the design resistance of the stress of the whole length of the weld.
The equivalent stress in the weld diagram shows the following stress:
Butt welds
Welds can be specified as complete joint penetration (CJP) butt welds or partial penetration (PJP) butt welds.
Partial penetration butt welds are checked in the same way as fillet welds (EN 1993-1-8:2005 – 4.7.2; EN 1993-1-8:2024 – 6.7.2).
Complete joint penetration butt welds are assumed to have the design resistance of the weaker of the connected parts (EN 1993-1-8:2005 – 4.7.1; EN 1993-1-8:2024 – 6.7.1(1)) and are not checked. This assumption is not valid in two cases. In these cases, the weld is automatically changed to the weld type CJP weld (checked), and the user is informed by a message in the operation that created the weld:
- The plate connected by its edge has a higher yield strength than the plate connected by its surface (both editions). The weld cannot be assumed to be as strong as the stronger of the plates. The weld is checked by the standard weld check (EN 1993-1-8:2005 – Formula (4.1); EN 1993-1-8:2024 – Formula (6.1)).
- At least one of the connected plates is made of steel grade higher than S460 ( MPa; EN 1993-1-8:2024 only). The weld is checked according to EN 1993-1-8:2024 – 6.7.1(2), Formula (6.7). A filler material from EN 1993-1-8:2024 – Table 6.2 must be chosen; with any other weld material, an error is issued and the calculation does not run.
where:
- – ultimate strength of the weaker of the connected plates
- – ultimate strength of the filler material (EN 1993-1-8:2024 – Table 6.2)
- – equivalent stress in the weld, see Fillet welds
A CJP weld (checked) is modeled and calculated as a partial penetration butt weld with the throat thickness equal to the thickness of the plate connected by its edge. The throat thickness cannot be edited. The conversion is re-evaluated every time the connection is regenerated, so it always follows the current steel grades in the model.
CJP butt welds between two plates connected edge to edge are not converted and are not checked. Only a detailing warning is issued.
Detailing
The detailing checks of welds depend on the weld type:
| Detailing check | Fillet weld | PJP butt weld | CJP weld (checked) |
| Minimum plate thickness | yes | yes | yes |
| Minimum throat thickness | yes | yes | – |
| Maximum throat thickness in a lap joint | single-sided only | – | – |
| Recommended minimum throat thickness | yes | – | – |
| Minimum throat thickness for ductility | yes | – | – |
| Maximum ultimate strength of the weld | yes | yes | yes |
| Minimum ultimate strength of the filler material | yes | yes | yes |
CJP butt welds that are not checked get a detailing check when two plates are connected edge to edge and the thinner plate has higher ultimate strength:
"CJP welds are not checked. Their resistance is assumed to be the same as that of the connected plate. Connected plates have different ultimate strength. CJP weld may fail at the interface of the weaker connected material."
Minimum plate thickness. The thickness of plates connected by welds is checked. An error is issued when the requirement is not satisfied:
- For hollow steel sections, the plate thickness should be at least 2.5 mm. For other plates, the plate thickness should be at least 4 mm (EN 1993-1-8:2005 – 4.1(1))
- For hollow steel sections, the plate thickness should be at least 1.5 mm (EN 1993-1-8:2024 – 9.1(3))
- For other plates, the plate thickness should be at least 3 mm (EN 1993-1-8:2024 – 4.1.2(2))
Minimum throat thickness. The throat thickness of fillet welds and partial penetration butt welds should be at least 3 mm according to EN 1993-1-8:2005 – 4.5.2(2) and EN 1993-1-8:2024 – 6.5.2(2). An error is issued when this requirement is not satisfied.
According to EN 1993-1-8:2024 – 9.5(2) and (3), the design throat thickness may be less than 3 mm if the welds are designed to have a higher design resistance per unit length of the hollow cross-section perimeter. This exception has not yet been developed.
Maximum throat thickness in a lap joint. The throat thickness of a single-sided fillet weld in a lap joint is limited by the thickness of the plate connected by its edge. An error is issued; such a weld is not feasible due to geometric constraints.

Recommended minimum throat thickness. A warning is issued when the throat thickness of a fillet weld is smaller than the recommendation in DIN EN 1993-1-8:2005 – NA to 4.5.2:
where:
- – weld throat thickness
- – thickness of the thicker connected plate
- units must be in [mm]
Minimum throat thickness for ductility. Information is issued when the throat thickness is smaller than the requirement for minimum ductility of welded joints in EN 1993-1-8:2024 – 6.9(4). The requirement is checked for both editions. For double-sided fillet welds:
where:
- – weld throat thickness
- – thickness of the plate connected by edge
- – weld correlation factor
- – safety factor for bolts and welds; editable in Code setup
- – plate yield strength
- – weld ultimate strength
- – safety factor for plates; editable in Code setup
The weld throat thickness for single-sided fillet weld is twice larger than that for double-sided fillet weld.
Maximum ultimate strength of the weld. Welds between parts with different strength grades should be designed using the properties of the material with the lower strength grade (EN 1993-1-8:2005 – 4.5.3.2; EN 1993-1-8:2024 – 6.5.3.2(5)). An error is issued when the ultimate strength of the weld material is higher than the ultimate strength of the weaker connected plate.
Minimum ultimate strength of the filler material. If a filler material from EN 1993-1-8:2024 – Table 6.2 is chosen, but the weld is checked by the standard weld check (Formula (4.1) or (6.1)), the filler material strength is not used in the check. In this case:
- an error is issued if the ultimate strength of the filler material is lower than the ultimate strength of the connected plates, because the check would overestimate the weld resistance (EN 1993-1-8:2024 – 6.2(2)),
- otherwise, information is issued that the filler material is disregarded.